The Jackdaw
New Member
I am a beginner and my first lettering on a vehicle has gone badly. One-Shot paint and very little thinning with white spirit. No hardener used.
Painted outdoors (9C/48F during the day) with very high humidity at night.
After 4 days, the paint had a nice gloss (so I believed I gave it enough time to dry before nightfall) and appeared hardened however it can be rubbed off easily with a dry cloth.
Is this due purely to the temperature/humidity of application or is there something else at play here?
I want to make sure I learn what I have done wrong before trying to find a heated workshop and start from scratch.
The van is a metallic silver and I made sure the area was clean and dry before starting.
Thanks
Painted outdoors (9C/48F during the day) with very high humidity at night.
After 4 days, the paint had a nice gloss (so I believed I gave it enough time to dry before nightfall) and appeared hardened however it can be rubbed off easily with a dry cloth.
Is this due purely to the temperature/humidity of application or is there something else at play here?
I want to make sure I learn what I have done wrong before trying to find a heated workshop and start from scratch.
The van is a metallic silver and I made sure the area was clean and dry before starting.
Thanks